Physical | Dry | Conditioned | Unit | Test Method |
Density | 1.40 | — | g/cm³ | ISO 1183 |
Molding Shrinkage
Across Flow : 73°F, 0.0787 in |
0.90 |
— |
% |
ISO 294-4 |
Flow : 73°F, 0.0787 in | 0.40 | — | % | |
Water Absorption (73°F, 24 hr) | 0.80 | — | % | ISO 62 |
Water Absorption (Equilibrium, 73°F, 50% RH) | 1.7 | — | % | ISO 62 |
Mechanical | Dry | Conditioned | Unit | Test Method |
Tensile Modulus (73°F) | 1.54E+6 | 1.15E+6 | psi | ISO 527-2 |
Tensile Stress (Break, 73°F) | 29700 | 21000 | psi | ISO 527-2 |
Tensile Strain (Break, 73°F) | 3.0 | 5.0 | % | ISO 527-2 |
Flexural Modulus (73°F) | 1.48E+6 | 943000 | psi | ISO 178 |
Flexural Stress (73°F) | 42100 | 29000 | psi | ISO 178 |
Poisson’s Ratio | 0.40 | — | ISO 527-2 | |
Impact | Dry | Conditioned | Unit | Test Method |
Charpy Notched Impact Strength
-22°F |
4.8 |
5.7 |
ft·lb/in² |
ISO 179 |
73°F | 5.2 | 6.7 | ft·lb/in² | |
Charpy Unnotched Impact Strength
-22°F |
33 |
40 |
ft·lb/in² |
ISO 179 |
73°F | 38 | 43 | ft·lb/in² | |
Notched Izod Impact Strength
-22°F |
4.8 |
5.7 |
ft·lb/in² |
ISO 180 |
73°F | 5.7 | 6.7 | ft·lb/in² | |
Thermal | Dry | Conditioned | Unit | Test Method |
Heat Deflection Temperature
66 psi, Unannealed |
500 |
— |
°F |
ISO 75-2/B |
Heat Deflection Temperature
264 psi, Unannealed |
482 |
— |
°F |
ISO 75-2/A |
Melting Temperature | 500 | — | °F | ISO 11357-3 |
CLTE – Flow (73 to 131°F, 0.0787 in) | 1.2E-5 | — | in/in/°F | ISO 11359-2 |
CLTE – Transverse (73 to 131°F, 0.0787 in) | 5.9E-5 | — | in/in/°F | ISO 11359-2 |
RTI Elec
0.0295 in |
248 |
— |
°F |
UL 746 |
0.0591 in | 248 | — | °F | |
0.118 in | 248 | — | °F | |
RTI Imp
0.0295 in |
212 |
— |
°F |
UL 746 |
0.0591 in | 212 | — | °F | |
0.118 in | 221 | — | °F | |
RTI Str
0.0295 in |
257 |
— |
°F |
UL 746 |
0.0591 in | 257 | — | °F | |
0.118 in | 257 | — | °F |
Specification: NYLON66+GF-ASCEND-Vydyne R533
|